E41-609 · Bearing Selection · Field Maintenance of a Worn Bearing Shaft Diameter · ★★★★
After the bearing seat of a drive shaft wore (Φ80mm → Φ79.5mm, depth 0.5mm), the maintenance worker restored the dimension by arc welding up the surface and machining it back, but the bearing loosened after only one month of use.
The worn journal was repaired by arc welding (manual arc welding with a J422 electrode), leaving a weld overlay about 3mm thick, and the Φ80mm dimension was restored by machining after welding. The problems are: (1) the hardness of the overlay is uneven (soft spots at HRC15~25), and under the compressive stress of the interference fit these soft spots deform plastically, so the interference falls from a mean of 0.03mm to 0.01mm; (2) micro-cracks (welding hot cracks) exist at the fusion line between the overlay and the base metal and propagate under alternating load, loosening the fit between the bearing inner ring and the journal; (3) the surface roughness of the journal after welding is Ra6.3μm (as machined), far above the required Ra0.8μm, so the actual interference is crushed at the microscopic peaks and the effective interference is insufficient. The effective interference between the bearing inner ring and the journal after the repair was only 0.008mm (originally designed 0.03mm), and the joint loosened after one month.
1) The preferred repair for a worn journal is thermal spraying (HVOF or plasma spray, with a uniform coating hardness of HRC55~60 and a bond strength >70MPa);
2) Or use electroplating repair (a hard coating with controllable thickness, Ra as low as 0.4μm);
3) Weld build-up repair is only suitable for non-fit surfaces or rough surfaces (precision grinding is required after welding);
4) After repair, check the hardness and roughness (HRC≥55, Ra≤0.8μm);
5) For emergency repairs use a split plummer block housing with a replaceable bore liner (the liner is exchanged directly).
FT_Bearing Design Handbook