Weld Repair of a Cracked Gearbox Housing Causes Secondary Deformation (Improper Repair)

E41-564 · Gearbox & Coupling Selection · Gearbox Housing Crack Weld Repair · ★★★

Problem Symptom

A crack (about 50mm long) appeared in a gearbox housing (HT250) and was repair welded. After welding a new crack (about 20mm long) appeared near the original crack and the housing deformed by 0.1mm.

Root Cause

When repair welding the HT250 cast iron housing the preheat was insufficient (only to 100℃) and a Z308 electrode (pure nickel cast iron electrode) was used. The welding heat input (about 15kJ/cm) raised the temperature in the weld zone to about 600℃, creating a steep temperature gradient between the surrounding HT250 parent material at 600℃ and the 100℃ preheat temperature. The thermal stress is σ_th=E×α×ΔT=130000×10×10⁻⁶×500≈650MPa (130GPa being the elastic modulus of cast iron, α=10×10⁻⁶/℃, ΔT=500℃). The tensile strength of HT250 is about 250MPa, so 650MPa far exceeds the strength of the material; stress concentrates at the crack tip and the crack propagates (the new crack extends about 20mm from the original crack tip along the heat-affected zone). At the same time the housing deforms by about 0.1mm as the stress is relieved, and the coaxiality of the bearing bores degrades from 0.02mm to 0.08mm.

Correct Solution

1) Cast iron housing repair welding procedure: preheat to 300~400℃ (overall heating) → weld with low current → cool slowly (furnace cool to 100℃);
2) Use Z408 or Z508 electrodes (pure nickel / nickel iron, which bond well to cast iron);
3) Stress-relief anneal at 500℃ after welding (to remove the welding stress);
4) Re-machine the bearing housing bores after welding (restoring the coaxiality to ≤0.02mm);
5) If the crack is not in a critical area (not in the bearing bore region), stop the crack by drilling (Φ3mm holes at both ends of the crack) and fill with epoxy resin.

Checklist

References

FT_13_Gearbox and Motor Matching Selection

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL