E41-765 · Other Selection · Steam Flange Leakage · ★★★
A steam pipeline (200 ℃, 1.5 MPa) flange (DN100, PN16) used a PTFE gasket and leaked after only 1 day.
At 200 ℃ the PTFE gasket creeps (cold flow); compression rate rises from 10% to 40% (4×), thickness drops from 3 mm to 2 mm. Bolt preload drops from initial 10 MPa to 3 MPa (70% relaxation); sealing stress 3 MPa < the required minimum 5 MPa → leakage. PTFE allowable operating temperature ≤150 ℃ long term, up to 260 ℃ short term, but at 200 ℃ the creep rate is high (about 0.02 mm/h); after 24 h creep is 0.48 mm (gasket thinned 16%), and sealing fails.
① Recheck all parameters per correct selection specifications
② Confirm that operating loads, environment, and service life all meet design requirements
③ Select reliable brands and appropriate models
④ Verify installation and operating conditions
⑤ Perform periodic inspection and maintenance after commissioning
FT_Machine Design Handbook