E41-612 · Gear Drive Selection · Open Gear Drive (ball mill) · ★★★★
The ball mill open gear (large gear m = 20, Z = 168) developed extensive tooth-surface pitting after 6 months of operation; the pits were 2–5 mm in diameter and 0.5–1 mm deep.
The pinion and gear tooth-surface hardness design was: pinion (40Cr, HRC50–55), gear (ZG35CrMo, HB240–280), hardness difference HBW (550 − 260 = 290). Per the design code, the open-gear hardness difference should be within HBW 50–100. The actual difference of 290 far exceeded the recommendation, so the pinion's hard tooth surface caused scraping wear on the gear's soft tooth surface. During meshing, the gear tooth surface was continuously scraped by the pinion's hard asperities; the contact stress σ_H = ZE×ZH×Zε×√(F_t×K×(u+1)/(b×d₁×u)) = 189.8×2.5×0.87×√(280000×2.0×(5.1)/400×400×5.1) ≈ 680 MPa. For ZG35CrMo (HB260), the contact fatigue limit σ_Hlim ≈ 550 MPa; actual σ_H = 680 > 550 MPa, exceeding the fatigue limit by 24%. Meanwhile, poor lubrication (the open gear was only coated with grease) caused the mesh-zone oil film to break, metal-to-metal contact → adhesion → tearing → pitting. After 6 months, pitting covered 30% of the tooth surface and the gear failed.
① The hardness difference between pinion and gear of an open gear should be controlled within HBW 50–100\n② Pinion hardness HRC45–50 recommended, gear HB280–320\n③ Or make pinion and gear hardness similar (e.g. both quenched-and-tempered plus tooth-surface hardened)\n④ Open gears must be equipped with an automatic lubrication device (spray lubrication, once per revolution)\n⑤ Strengthen sealing and dust protection (prevent dust from entering the mesh zone and worsening wear)
FT_Gear Transmission Design