E41-617 · Gear Transmission Selection · Precision Gear Transmission (Grade 6) · ★★★★
For the precision gear (grade 6 accuracy, m=2 mm, 20CrMnTi carburized and hardened), the tooth-profile error worsened from 0.005 mm to 0.025 mm after heat treatment, exceeding the grade 6 requirement (0.008 mm).
The gear underwent thermal distortion during carburizing and hardening (930℃ carburizing → 830℃ quenching → 200℃ tempering). The main sources of distortion: ① during carburizing the gear underwent a structural transformation (austenitization) at high temperature (930℃), with a volume change of about +4%; ② during quenching the austenite → martensite transformation caused a volume expansion of about +4%; ③ the non-uniform cross-section led to inconsistent cooling rates (fast at the tooth tip, slow at the root), producing non-uniform phase transformation and thermal stress. The gear outer diameter grew from Φ50 mm to Φ50.12 mm (0.24%), and the bore grew from Φ20 mm to Φ20.08 mm (0.4%). The cumulative pitch error increased from 0.006 mm before heat treatment to 0.020 mm. The distortion came mainly from the way the gears were placed (flat placement causing self-weight deformation plus the stacking pressure of gears above and below). After heat treatment the gear could no longer be corrected to grade 6 accuracy by grinding (the grinding allowance was only 0.05 mm per side, insufficient to eliminate the 0.02 mm cumulative pitch error).
① Precision gears should use press quenching for heat treatment (the gear is held under pressure in a die during quenching to limit distortion)\n② Add stress-relief annealing before carburizing (650℃×2 h, to eliminate machining stresses)\n③ Place the gears upright in the furnace (fixed on a mandrel, to avoid self-weight distortion and stacking pressure)\n④ Provide sufficient grinding allowance (≥0.15 mm per side for precision gears)\n⑤ Add a stabilizing treatment after heat treatment (160℃×8 h aging, to stabilize retained austenite)
FT_Gear Transmission Design