Knowledge Base › Selection Error Cases › Early wear of the worm wheel caused by improper material selection for the worm drive (worm reducer)

Early wear of the worm wheel caused by improper material selection for the worm drive (worm reducer)

E41-627 · Gear Transmission Selection · Worm Reducer · ★★★★

Problem Description

After 3 months of operation a worm reducer (center distance 160 mm, ratio 40:1) showed a drop in output torque; inspection found that the worm-wheel tooth thickness had worn by 0.5 mm (original tooth thickness about 3 mm).

Root Cause

The worm wheel material was ZCuSn10Pb1 (tin bronze), the worm material was 40Cr (tooth surface hardened to HRC50), and the worm was ground. The lubricating oil was VG320 mineral oil. The worm speed n1=1450 rpm, the worm-wheel speed 36.25 rpm, and the sliding velocity v_s=π×d₁×n₁/(60000×cosγ)=3.14×50×1450/(60000×cos5.7°)=3.8 m/s. The worm-wheel contact stress σ_H=ZE×√(K×T₂/(d₁×d₂×b₂))=160×√(1.5×900/(50×200×35))≈90.7 MPa. The allowable contact stress of tin bronze is [σ_H]≈150 MPa (at vs=3.8 m/s). However, the actual wear rate (tooth-thickness wear) was about 0.17 mm/month, far higher than the normal wear rate (about 0.01 mm/month). The cause was that the lubricating oil was contaminated with residual abrasive particles from grinding the worm (SiC, particle size 10~50 μm), because the worm was not thoroughly cleaned after grinding. The SiC particles (hardness HV2600) embedded in the soft worm-wheel tooth surface (HB90) and in turn abraded the worm tooth surface. As the worm tooth surface became rough from abrasive wear, it further accelerated the worm-wheel wear. Incomplete cleaning of the reducer housing → residual abrasive particles → a vicious cycle of abrasive wear → the worm wheel was scrapped after 3 months.

Corrective Solution

① The housing must be thoroughly cleaned before assembling the worm drive (flush 3 times with kerosene or a cleaning agent)\n② After grinding, the worm must be demagnetized and ultrasonically cleaned (to remove abrasive particles embedded in the tooth surface)\n③ It is recommended to upgrade the worm-wheel material to ZCuSn12Ni2 (nickel-containing tin bronze, 30% better wear resistance)\n④ Use a worm-drive-specific oil for lubrication (containing extreme-pressure EP additives, to reduce wear)\n⑤ Replace the lubricating oil after the first 200 h of running (to discharge the initial running-in abrasive particles)

Checklist

Reference

FT_Gear Transmission Design

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL