E41-728 · Seal Component Selection · Mechanical Seal Wear · ★★★★
A water pump mechanical seal (carbon vs. silicon carbide) leaked after 2 months; the stationary ring (carbon) wore 2 mm deep (allowable 1 mm).
The pump circulated water containing fine sand (particle concentration about 50 mg/L, size 10–50 μm). The mechanical seal's friction pair was carbon (soft, easy to wear) against silicon carbide (hard). Sand grains (HV1000) embedded in the carbon seal face (HB80) and ground against the silicon carbide face (HV2500) as it rotated. The grains formed abrasive wear between the faces; wear rate Q=K×F×v/H (K=10⁻⁴, F=100 N, v=5 m/s, H=800 MPa), calculated wear ≈6×10⁻⁴ mm³/s, and the carbon face wore about 0.3 mm per month. After 2 months the carbon ring wore 0.6 mm (design allowable 1 mm), within limit. But the silicon carbide ring also wore under the grains (0.02 mm/month); seal face flatness degraded from 0.3 μm to 1.5 μm, exceeding flatness limits and causing leakage.
① Verify seal selection against sealing conditions (pressure/temperature/media/speed)
② Confirm material and hardness meet requirements
③ Control journal roughness and runout to prevent eccentric wear
④ Install correctly (lubricate the lip, prevent reverse installation)
⑤ Periodically inspect and replace on schedule
FT_Seal Spring Design