E41-729 · Seal Component Selection · Flange Seal Leakage · ★★★
A steam pipe flange (DN100, PN16, 250°C) used an asbestos-rubber gasket; after 1 week steam leaked at the gasket.
The asbestos-rubber gasket (XB450, 3 mm thick) at 250°C saw compression increase from 20% to 35% (continuous creep); residual stress dropped from the initial 10 MPa to 3 MPa (stress relaxation about 70%). Flange bolt preload at hot state (250°C) rose due to bolt thermal expansion (Q235, α=12×10⁻⁶/°C), but relaxation of the flange (HT250) and gasket (asbestos rubber) left insufficient effective sealing stress. When gasket residual stress 3 MPa< minimum sealing stress 5 MPa, a gap formed between gasket and flange face → leakage. Correct selection: use a spiral-wound gasket (304 stainless + graphite ribbon, rated to 650°C, creep <0.1%), whose stress relaxation at 250°C is only 5%.
① Verify seal selection against sealing conditions (pressure/temperature/media/speed)
② Confirm material and hardness meet requirements
③ Control journal roughness and runout to prevent eccentric wear
④ Install correctly (lubricate the lip, prevent reverse installation)
⑤ Periodically inspect and replace on schedule
FT_Seal Spring Design