E42-007 · Fatigue Fracture · CNC Lathe Spindle · ★★★
Fracture at the shoulder after 14 months of running, machine stopped
[Stress Concentration] With shoulder radius r=1mm and d/D=0.8, the theoretical stress concentration factor is Kt≈2.4; at a nominal stress σ_n=120MPa the local stress reaches 288MPa.
[Fatigue Accumulation] The quenched-and-tempered material has σ_b=750MPa and σ-1=340MPa. The effective stress amplitude σ_a=288×Ka×Kb=260MPa exceeds the corrected endurance limit of 210, giving a life of N=1.2e7 cycles, about 14 months.
[Design Omission] No R≥0.1d transition was provided and no shot peening was applied, so the spindle fractured.
1) Increase the shoulder fillet radius to R4 (≥0.1d);
2) Apply roller burnishing / shot peening at the fillet;
3) Verify by finite element that the fatigue life is ≥10 years;
4) Change the material to 41Cr4 quenched and tempered with magnetic-particle flaw detection;
5) Add monitoring at the critical section;
6) Run a fatigue bench test on the first shaft article;
7) Establish a life dossier for critical shafts;
8) Include fillet reinforcement in the shaft design guidelines.
GB/T 3075-2008 Metallic Materials — Fatigue Testing