E42-009 · Fatigue Fracture · Flange Coupling Disc · ★★
Cracking and leakage at the edge of an M16 bolt hole after 80000 load cycles
[Hole-Edge Stress Concentration] The hole edge has no chamfer, Kt≈3.0, and the bolt preload induces a hole-edge stress σ=3×90=270MPa.
[Fatigue Initiation] The stress amplitude σ_a=270MPa exceeds the hole-edge fatigue limit of 180MPa, so a crack initiates after N_f=8e4 cycles.
[Design Omission] The hole mouth was not chamfered C1 and no flaw detection was performed.
1) Chamfer the hole mouth C1 and polish it;
2) Provide an R-arc transition at the hole edge;
3) Raise the roughness of the coupling disc face to Ra1.6;
4) Check the bolt preload against VDI 2230;
5) Apply magnetic-particle inspection to the hole edge;
6) Perform fatigue verification of load-bearing flanges;
7) Assemble with a torque wrench to a specified torque;
8) Include leakage patrol inspection and torque-controlled assembly in the maintenance specification.
VDI 2230 High-Strength Bolted Joints