T-Joint Without a Bevel Causes Fatigue Cracking at the Weld Toe

E42-109 · Fatigue Fracture · Port Crane Main Girder · ★★★

Problem Symptom

Fatigue cracks at the weld toe of the T-section stiffener after 1.8e6 cycles, the main girder leaks water

Root Cause

[Toe Stress Concentration] The T-joint uses a fillet weld without a bevel, giving a toe stress concentration Kt=2.4. With an alternating stress σ=80MPa in the main girder, σmax=192MPa.
[Fatigue Accumulation] 192MPa is close to the girder steel fatigue limit σ-1=180MPa, so cracking occurred after 1.8e6 cycles.
[Design Omission] The T-joint had no bevel, the weld toe was not ground and the fatigue was not checked.

Correct Solution

1) Change the T-joint to a full penetration weld with a bevel;
2) Grind the weld toe to R1.5;
3) Carry out a hot-spot stress fatigue check by finite element;
4) Add longitudinal stiffening ribs to the main girder;
5) Inspect every weld by UT;
6) Perform magnetic-particle inspection after 1.5e6 cycles;
7) Seal against water ingress with corrosion protection;
8) Include weld toe fatigue in the specification.

Checklist

References

GB/T 3811 Code for Design of Cranes