E42-157 · Fatigue Fracture · Vibrating Screen M24 Bolt · ★★★
After 3 months of operation the bolt fractures; fracture at first engaged thread.
[Alternating Stress] Equipment vibration subjects bolt to axial alternating σ_a=120MPa exceeding 10.9 grade fatigue limit. [Root Concentration] Thread minor diameter K_t=3.2; actual σ_max=384MPa. [Design Omission] Preload not controlled; no fine thread enlarged nut; 60 sets fracture per year.
1. Change bolt to fine thread M24×2 to reduce stress amplitude.
2. Set preload torque at 0.7σ_s and torque to specification.
3. Add disc spring washer under nut.
4. Thread engagement length ≥1.5d.
5. Improve surface quality to Ra1.6 to reduce source.
6. Switch to grade 12.9 and roll threads.
7. Sampling inspect preload decay every 3 months.
8. Dual visual + magnetic-particle inspection at fracture-prone positions.
GB/T 3098.1-2010