E42-159 · Fatigue Fracture · Port Crane Jib Cruciform Node · ★★★
After 2 years, node web weld root crack 40mm, extending to base metal.
[Lack of Fusion] Double-sided welding of cruciform joint without back-gouging; lack of fusion 3mm deep. [Stress Concentration] Weld root sharp corner K_t=2.8; hot spot stress σ=180MPa. [Design Omission] Not checked per node fatigue Detail; no double-sided groove; crack caused 15-day shutdown.
1. Machine double-sided K-groove on cruciform node.
2. Weld one side, back-gouge, then weld.
3. Control stress by fatigue Detail classification.
4. UT inspect weld root for lack of fusion.
5. Add reinforcement plate at node outer edge to lower stress.
6. Post-weld stress-relief annealing to eliminate residual stress.
7. Bond strain gauges at crack-prone positions for stress monitoring.
8. Magnetic-particle inspect nodes every 2 years.
GB 50017-2017