Knowledge Base › Structural Design Error Case Study › Cast Steel Weld Repair Insufficient Preheat Causing Cold Cracks

Cast Steel Weld Repair Insufficient Preheat Causing Cold Cracks

E42-219 · Welding Deformation and Defects · Excavator Arm Cast Steel · ★★★

Problem Description

Delayed crack 60mm long appears 24h after weld repair.

Root Cause

[Insufficient Preheat] Cast steel ZG270 weld repair zone not preheated; cooling rate > critical; hydrogen cannot escape. [Cold Crack] Residual hydrogen + constraint stress cause 60mm delayed crack. [Design Omission] No preheat temperature specified; no low-hydrogen electrode.

Corrective Solution

1. Preheat to 150℃ before welding.
2. Use low-hydrogen electrode E5015 baked at 350℃.
3. Wrap with insulation blanket for slow cooling after welding.
4. Grind weld repair zone smooth transition.
5. Magnetic-particle inspection 48h after welding.
6. Control ambient humidity ≤80%.
7. Sample delayed cracks each batch.
8. Stress-relief anneal critical parts after welding.

Checklist

Reference

GB/T 9443-2019