E42-388 · Welding Deformation and Defects · PC200 Boom Main Weld · ★★★
PC200 boom main weld HAZ crack 40mm; arm-break risk; 1 unit repaired per month
[Cold Crack] High-strength steel hardenability; hydrogen crack without preheat.
[Break Risk] Main weld load-bearing fails.
[Design Omission] No preheat; no low-hydrogen welding; safety factor 1.3.
1) Preheat 120℃ before welding;
2) Bake low-hydrogen electrode;
3) Post-weld dehydrogenation;
4) UT inspect weld;
5) Flaw detect each arm;
6) Upgrade base metal grade;
7) Post-weld annealing;
8) Periodic patrol.
GB/T 9139-2018