E42-460 · Welding Deformation and Defects · Vertical Storage Tank Wall Plate · ★★
5000m³ tank wall plate vertical seam angular distortion 12mm exceeds allowable 3; angular misalignment out of tolerance; 2 repairs per month
[Angular Distortion] Single-side weld heat input q=28kJ/cm; uneven transverse shrinkage gives angular distortion 12mm.
[Angular Misalignment] Caused by misaligned edge.
[Design Omission] No double-sided symmetric welding; no reverse deformation; safety factor 1.4 (should be ≥2.0).
1) Change to double-sided symmetric welding;
2) Add 8mm reverse deformation;
3) Control heat input ≤20kJ/cm;
4) Add copper backing strip;
5) Measure angular distortion per seam;
6) Control angular misalignment ≤3mm;
7) Straighten after welding;
8) Periodic re-measurement.
GB/T 50128-2014