Pouring Temperature Too Low Causes Cold Shuts and Leakage in a Cast Iron Housing

E42-063 · Casting Defects · Cast Iron Housing HT250 · ★★

Problem Symptom

Cold shut in the thin wall, leakage at a water pressure of 0.4MPa

Root Cause

[Pouring Temperature] The pouring temperature is 1280℃ (1360℃ required), so the fluidity is poor and in the thin wall of 6mm far from the gate the metal front freezes early.
[Cold Shut] Two metal streams fail to fuse and leave a seam, which leaks at a water pressure of 0.4MPa.
[Design Omission] The pouring temperature was not controlled and no overflow was added at the thin wall, so the part leaked and had to be reworked.

Correct Solution

1) Raise the pouring temperature to 1340-1380℃;
2) Add overflow risers at the thin wall;
3) Increase the cross-section area of the gating system;
4) Optimise the mould sand permeability;
5) Carry out a hydrostatic test at 0.6MPa;
6) Repair and grind the cold shut;
7) Freeze the pouring temperature on the process sheet;
8) Include the pouring temperature in the first-article confirmation.

Checklist

References

GB/T 9439-2010 Grey Iron Castings