Abrupt Wall Thickness Change and High Sulphur Content Cause Hot Tearing and Leakage in the Casting

E42-114 · Casting Defects · Diesel Engine Block Cast Iron · ★★

Problem Symptom

Hot cracks at the corner of the water outlet, leakage in the pressure test, 5% of the batch affected

Root Cause

[Hot Tearing Mechanism] At the water outlet corner the wall thickness changes abruptly and the elevated sulphur and phosphorus content raise the hot brittleness, so restrained shrinkage in the late solidification stage produces hot tears.
[Crack Formation] The shrinkage stress at the corner exceeds the strength of the weak grain boundaries and the part cracks.
[Design Omission] No fillet transition was provided and the sulphur and phosphorus content was not controlled.

Correct Solution

1) Add an R8 fillet and a uniform wall transition at the corner;
2) Control the sulphur and phosphorus content at S≤0.06% and P≤0.08%;
3) Provide anti-tearing ribs to spread the shrinkage;
4) Raise the pouring temperature to reduce cold shuts;
5) Pressure test 100% and mark the parts;
6) Radiographically inspect the crack-prone areas;
7) Perform rapid furnace-side chemical analysis;
8) Include the hot tearing risk in the casting process.

Checklist

References

GB/T 9439 Grey Iron Castings