Graphite Flotation in Ductile Iron Causes Low Strength and Chunking of the Hub Surface

E42-113 · Casting Defects · Wind Turbine Casting Hub · ★★

Problem Symptom

Graphite clusters and low hardness on the upper surface of the hub, chunks break off after machining

Root Cause

[Graphite Flotation] A high pouring temperature and a high carbon equivalent let graphite float and cluster at the surface, distorting the matrix.
[Strength Reduction] The surface nodularity is <70% and the hardness is 20% lower, so chunks break off at the load-carrying areas.
[Design Omission] The gating system had no slag trap and the carbon equivalent was out of control.

Correct Solution

1) Control the carbon equivalent CE≤4.5;
2) Lower the pouring temperature to 1350±20;
3) Fit a slag trap and a skimming gate;
4) Strengthen the nodularising inoculation treatment;
5) Inspect the surface 100% by UT and hardness;
6) Increase the machining allowance to stay clear of the surface layer;
7) Re-test the mechanical properties on cast-on test coupons;
8) Include the nodularity in the acceptance.

Checklist

References

GB/T 1348 Ductile Iron Castings

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL