Excessive Pouring Speed Causing Sand Wash and Sand Holes with Casting Leakage

E42-163 · Casting Defects · HT250 Gearbox Housing · ★★

Problem Description

The housing leaks at 0.4MPa hydrostatic test; sectioning reveals sand holes Φ3mm.

Root Cause

[Sand Wash] Pouring speed v=1.2m/s exceeds the critical value, scouring the mold cavity into sand holes. [Air Entrainment] Turbulence entraps gas, causing subsurface porosity + sand holes. [Design Omission] No buffer in the gating system, speed not controlled.

Corrective Solution

1. Control pouring speed to ≤0.6m/s.
2. Add a buffer basin and slag filter in the sprue.
3. Add a slag trap at the end of the runner.
4. Keep molding sand permeability uniform, moisture 4-5%.
5. Raise pouring temperature to 1380℃ to favor venting.
6. Add vent channels in the cavity.
7. Leak-test the shell mold at 0.5MPa.
8. Section rejects and build a defect archive.

Checklist

Reference

GB/T 9439-2010

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL