Knowledge Base › Structural Design Error Case Study › Restrained Shrinkage of Heavy Sections Causing Hot-Tear Leakage

Restrained Shrinkage of Heavy Sections Causing Hot-Tear Leakage

E42-164 · Casting Defects · ZG270-500 Box · ★★

Problem Description

Cracks 30mm long at the box corner; leaks under hydrostatic test.

Root Cause

[Restrained Shrinkage] Abrupt wall thickness change, poor core collapsibility; solidification shrinkage is restrained, tensile stress σ=3MPa. [Hot Tear] Low-melting segregation at grain boundaries (S=0.035%) tears the liquid film. [Design Omission] No process ribs, S not controlled; crack rate 16%.

Corrective Solution

1. Add anti-crack process ribs at corners, thickness 1/3 of wall.
2. Use easily collapsible resin cores to reduce restraint.
3. Control base metal S, P to ≤0.025%.
4. Add chills at hot spots to balance solidification.
5. Place risers in the gating system to feed the corner.
6. Raise pouring temperature to 1420℃ to reduce hot tearing.
7. Slow cooling after casting to relieve thermal stress.
8. 100% leak inspection at 0.6MPa hydrostatic test.

Checklist

Reference

GB/T 11352-2009

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »