Early Freezing of Feeding Channel Causing Surface Sink

E42-165 · Casting Defects · QT600-3 Brake Drum · ★★

Problem Description

Depression 4mm deep on the drum face; sink-out at wall-thickness transitions is out of tolerance.

Root Cause

[Channel Blockage] The riser neck freezes too early, cutting off the feed channel; liquid feeding at the hot spot is insufficient. [Sink-out] The surface sinks 4mm; porosity appears after machining. [Design Omission] Riser neck not insulated, no exothermic riser used; sink rate 11%.

Corrective Solution

1. Add an insulating sleeve to the riser neck to delay freezing.
2. Switch to exothermic risers to raise feeding efficiency.
3. Place chills at hot spots for balance.
4. Size risers by modulus M≥1.2.
5. Raise pouring temperature to 1380℃.
6. Provide separate vent and feed channels.
7. NDT at sink-out locations.
8. Section the first piece to verify feeding.

Checklist

Reference

GB/T 1348-2019

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »