E42-221 · Casting Defects · Ductile Iron Valve Body · ★★★
At 0.6MPa hydrostatic test, 10% of valve bodies leak; sectioning reveals porosity.
[No Riser Feeding] No riser at the valve body hot spot; liquid feeding is insufficient during solidification. [Porosity Leakage] Interdendritic shrinkage cavities interconnect, leaking at 0.6MPa hydrostatic test. [Design Omission] Risers not laid out per balanced solidification, no chills used.
1. Place two Φ60 risers at the hot spot.
2. Add chills to control solidification sequence.
3. Control pouring temperature to 1360±20℃.
4. X-ray inspect the castings.
5. 100% batch pressure test.
6. Use mold flow analysis in process design.
7. Section each batch for porosity sampling.
8. Design knock-off riser necks.
GB/T 1348-2019