E42-222 · Casting Defects · Cast Iron Machine Bed · ★★★
After machining the guideway surface, dross holes Φ3~5mm are exposed; scrap rate 8%.
[Slag Trap Failure] No slag filter in the sprue and no slag trap in the runner; molten slag enters the cavity with the stream. [Dross Hole Defect] Dross holes on the guideway surface leave voids after finish machining. [Design Omission] Gating system not designed for slag trapping, no ceramic filter used.
1. Add a foam ceramic filter to the sprue.
2. Place two slag traps in the runner.
3. Add a slag weir in the pouring cup.
4. Use slag removal agent in melting and skim thoroughly.
5. Control flow rate for steady pouring.
6. 100% magnetic particle inspection of guideway surface.
7. Section each batch to check dross.
8. Control impurities in returns.
GB/T 9439-2010