E42-513 · Casting Defects · Cast Iron Bed (HT300) · ★★

Problem Description

Shrinkage cavity φ15 at the guideway root, leaking after machining; scrap rate 8%; 5 parts scrapped per month

Root Cause

[Shrinkage Cavity] Riser too small, feeding insufficient; solidification shrinkage leaves a φ15 cavity.
[Pouring] Low temperature, poor filling.
[Design Omission] No riser, abrupt wall jump; safety factor 1.3 (should be ≥2.0).

Corrective Solution

1) Enlarge the riser;
2) Provide chills;
3) Raise pouring temperature to 1380℃;
4) Check shrinkage cavities per heat;
5) Limit wall-thickness difference;
6) Insulate the riser;
7)NDE;
8) Periodic re-measurement.

Checklist

Reference

GB/T 9439-2010