Second Type Temper Embrittlement Causes Brittle Fracture of the Hammer Rod

E42-117 · Heat Treatment Distortion & Cracking · Air Hammer Rod 40Cr · ★★★

Problem Symptom

Impact energy dropped sharply after tempering at 500~550℃ followed by slow cooling, and the rod fractured in service

Root Cause

[Temper Embrittlement] When alloy steel is tempered at 500~550℃ and cooled slowly, P and Sb segregate at the grain boundaries and the impact toughness falls.
[Brittle Fracture] The room temperature impact energy Akv dropped from 60J to 18J and the part fractured in service.
[Design Omission] No fast cooling was applied to avoid the brittle temperature range.

Correct Solution

1) Oil cool or water cool after tempering to avoid the brittle temperature range;
2) Choose a tempering temperature outside 500~550℃;
3) Change to a Mo-series steel to suppress temper embrittlement;
4) Re-test the room temperature impact energy for every batch;
5) Control the grain boundary segregation chemistry;
6) Normalise after forging to refine the grain size;
7) Perform NDT before entering service;
8) Include temper embrittlement in the heat treatment specification.

Checklist

References

GB/T 3077 Alloy Structural Steels