Excessive Quenching Cooling Rate Causes Quench Cracking of the Gear Shaft

E42-116 · Heat Treatment Distortion & Cracking · Gearbox Gear Shaft 20CrMnTi · ★★★

Problem Symptom

Longitudinal cracks at the shaft shoulder after quenching, the whole batch scrapped

Root Cause

[Thermal Stress Superposition] With the cooling too fast, the transformation stress below Ms superimposes on the thermal stress and the axial tensile stress exceeds the fracture strength.
[Cracking] The stress peak at the abrupt shoulder section change causes a longitudinal crack.
[Design Omission] Stepped quenching was not used and there was no preheat.

Correct Solution

1) Change to stepped quenching (160℃ salt bath);
2) Preheat to 200℃ before quenching to reduce the temperature difference;
3) Add a fillet at the shoulder to reduce the abrupt section change;
4) Control the quench medium temperature;
5) Temper promptly after quenching;
6) Inspect every part for cracks by magnetic-particle and UT;
7) Sample the hardness gradient;
8) Include the quench cracking risk in the heat treatment process.

Checklist

References

GB/T 16923 Normalising and Annealing of Steel Parts

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL