E42-516 · Heat Treatment Distortion and Cracking · Drive Long Shaft (40Cr) · ★★
Long shaft φ80×2500 bends 1.2mm after quenching, exceeding the 0.3 allowance; straightening cracks; 4 shafts scrapped per month
[Quench Distortion] Uneven cooling; thermal stress causes 1.2mm bend.
[Cracking] Straightening stress superimposed on residual stress.
[Design Omission] Not vertically hung-quenched, not stress-relieved; safety factor 1.3 (should be ≥2.0).
1) Vertical hang-quench;
2) Martemper;
3) Temper promptly;
4) Measure bend on each shaft;
5) Limit lifting load;
6) Press quenching;
7) Stress-relief annealing;
8) Periodic re-measurement.
GB/T 16923-2008