E42-242 · Thermal Deformation and Thermal Stress · Thin-Wall Aluminum Housing · ★★★
After finish machining, housing roundness 0.08mm (allowance 0.03); rebounds after cooling.
[Cutting Heat] Surface speed v=300m/min; thin wall dissipates poorly; temp rise ΔT=40℃. [Thermal Distortion] Housing heats and rounds 0.08; rebounds out of tolerance after cooling. [Design Omission] Insufficient cooling; rough/finish not separated.
1. Separate rough/finish; finish allowance 0.3mm.
2. High-pressure coolant to flush chips.
3. Add process ribs to prevent distortion.
4. Control coolant temp 25℃.
5. Fully cool before finish cut.
6. Measure roundness each batch.
7. Contour support fixture.
8. Symmetric feed to reduce thermal bias.
GB/T 1800.2-2009