E42-497 · Impact and Overload Fracture · Press Die · ★★
Press (160t) die overload edge chipped; production stopped; 2 sets scrapped per month
[Overload] Plate thickness exceeded; blanking force F=2000kN exceeded die strength and chipped it.
[Chipping] Edge cracked.
[Design Omission] No material thickness limit, no protection; safety factor 1.3 (should be ≥2.5).
1) Limit plate thickness to ≤6mm;
2) Add guidance to the die cavity;
3) Provide overload protection;
4) Raise edge hardness;
5) Edge check each shift;
6) Limit blanking force;
7) Upgrade material to DC53;
8) Periodic re-measurement.
GB/T 10923-2009