E42-146 · Residual Stress Distortion · Spring Steel Strip Shot Peened · ★★
Double-side shot peening is uneven and the strip warps by 1.5mm
[Residual Stress Difference] Uneven shot peening intensity on the two sides produces asymmetric compressive residual stress in the surface layer and the strip bends.
[Warping] The stress difference warps the thin strip by 1.5mm.
[Design Omission] The peening intensity was not controlled and the two sides were not made consistent.
1) Control the shot peening intensity identically on both sides;
2) Calibrate the arc height with coupons;
3) Fit anti-warp tooling for thin strip machining;
4) Flatten the strip after peening;
5) Measure the residual stress by X-ray diffraction;
6) Inspect the warping 100%;
7) Freeze the process parameters;
8) Include the peening distortion in the process.
GB/T 18838 Shot Peening Equipment — General Specification