E42-196 · Residual Stress Deformation · Thin-wall aluminum alloy housing · ★★
After finish milling, wall thickness variation 0.08mm (allowable 0.03), deformed.
[Tool deflection] Thin-wall low stiffness, milling radial force caused 0.05mm tool deflection. [Deformation] Springback after unloading, wall variation 0.08. [Design Omission] No auxiliary support, no layered milling; high scrap rate.
1. Add auxiliary support inside thin wall.
2. Layered milling to reduce tool deflection.
3. Reduce milling parameters to lower radial force.
4. Use sharp tools.
5. Rough-slot first then finish mill.
6. Symmetric machining to equalize deformation.
7. On-line wall-thickness measurement after machining.
8. Re-position if deformation out of tolerance.
JB/T 5000.3-2007