E42-326 · Residual Stress Deformation · Welded thin-plate component · ★★
Welded thin plate (δ=3): post-weld warpage 5mm, flatness out of tolerance; 6 pieces scrapped monthly
[Residual stress] Welding longitudinal residual stress σ=250MPa, thin-plate warpage.
[Warpage] Angular distortion plus bending distortion.
[Design Omission] No symmetric welding, no peening for stress relief; safety factor only 1.3.
1) Double-sided symmetric welding;
2) Peen after each layer to relieve stress;
3) Pre-set 2° distortion compensation;
4) Rigid fixture clamping;
5) Post-weld annealing;
6) Flatness check each batch;
7) Optimize welding sequence;
8) Mechanical straightening.
GB/T 19869.1-2005