E43-619 · Surface roughness mismatched with the fit · A bonded joint designed Ra3.2 but measured Ra0.4, the over-smooth surface gives poor adhesive anchoring and the joint disbonds in shear · ★★
The bonding surface at Ra0.4 is too smooth; the adhesive has insufficient mechanical anchoring, and the interface disbonds under shear load.
[Mechanism] Structural bonding relies on wetting and micro-anchoring by the adhesive; an over-smooth surface offers few anchoring sites, so interface shear strength is low and disbonding is likely.
[Calculation] At Ra0.4 the anchoring area is insufficient, bond shear strength drops about 40% versus a Ra3.2 sandblasted surface, and disbonding occurs under overload.
[Design Omission] The bonding surface is over-smooth and not sandblasted, a design defect → insufficient anchoring and disbonding.
1) Sandblast the bonding surface to Ra3.2~6.3 to increase anchoring;
2) Set roughness per the adhesive process;
3) Degrease and activate before bonding;
4) On the first article, verify Ra and shear strength;
5) Specify bonding-surface Ra and sandblasting on the drawing;
6) Control the bond-line thickness;
7) Meet cure temperature and pressure;
8) Verify by a shear test.
GB/T 131-2006 Geometrical product specifications — Surface texture designation