E43-637 · Surface Roughness Mismatch with Fit · A crankshaft main journal designed Ra0.2 but measured Ra0.8, causing rapid bearing wear, oil-film breakdown and bearing burnout · ★★★
The crankshaft journal is too rough at Ra0.8; the bearing soft layer is abraded, the oil film breaks down, peak contact causes bearing burnout and seizure.
[Mechanism] The crankshaft journal slides against the bearing; excessive roughness abrades the bearing like an abrasive and breaks the oil film, and peak contact overheats into bearing burnout.
[Calculation] With oil film h≈2μm, √(0.8²+Ra_bearing²) gives λ<1; peak contact raises the wear rate, and the bearing burns out within a few hundred hours.
[Design Omission] The journal was left too rough; this design defect causes bearing wear and burnout.
1) Grind/polish/superfinish the journal to Ra0.1~0.2;
2) Set journal Ra per plain-bearing requirements;
3) Control roundness and oil-hole chamfers;
4) Measure Ra and roundness on the first article;
5) Call out journal Ra on the drawing;
6) Keep oil passages clean;
7) Match clearance and oil grade;
8) Test bearing wear on a rig.
GB/T 131-2006 Geometrical product specifications — Surface texture designation