E43-690 · Taper and Angle Fit Error · Pressure-vessel groove designed V-type 60°±2.5° but measured 45°, giving a narrow groove, incomplete root penetration, and weld slag inclusions · ★★★
The weld groove angle was too small at 45° (designed 60°); the groove was undersized, the torch could not reach the root, the root was incompletely penetrated, and the weld had excessive slag inclusions.
[Mechanism] The weld groove angle ensures torch access and penetration depth; too small an angle narrows the groove, gives poor root fusion, and causes incomplete penetration and slag inclusions.
[Calculation] A 15° groove-angle error reduces the groove opening width by 40%, restricts torch weaving, leaves insufficient root penetration, and produces incomplete-penetration defects.
[Design Omission] The groove was machined at an out-of-tolerance angle; the design defect leads to incomplete penetration and slag inclusions.
1) Machine the groove to 60°±2.5°;
2) Check the angle with a groove template;
3) Ensure the root face and gap meet requirements;
4) Grind out the root before welding;
5) Inspect the first-article weld by NDT;
6) Keep the groove faces clean;
7) Specify the groove angle on the drawing;
8) Perform post-weld nondestructive testing.
GB/T 985.1-2008 Preparation of weld joints for gas welding and manual arc welding