E43-353 · Welded/Cast Forming Dimensional Error · A barrel 2000mm long, 200mm bore, designed bore 200±0.1, measured post-weld shrinkage 199.4 · ★★
Longitudinal shrinkage of the circumferential seam shortens the barrel by 1.2mm and shrinks the bore by 0.6mm, pushing the fit out of tolerance.
[Mechanism] Longitudinal cooling shrinkage of the circumferential seam shortens the barrel section and contracts it radially; the accumulation pushes bore and length out of tolerance.
[Calculation] Longitudinal shrinkage ΔL≈0.6mm/m×2m=1.2mm; radial shrinkage Δd≈ΔL·d/L=1.2×200/2000=0.12 (0.6mm measured after multiple seams accumulate).
[Design Omission] No weld-shrinkage allowance was left — a design defect leading to bore error.
1) Leave a shrinkage allowance of 1.5mm per 2000mm in the cut length;
2) Weld in segments with symmetric skip sequences to control shrinkage;
3) Mechanically finish the bore after welding;
4) Use internal support tooling to prevent radial shrinkage;
5) Control the welding sequence to reduce accumulation;
6) Temper after welding to relieve stress;
7) 100% inspect the bore with a bore gauge;
8) Measure first-article bore ≤0.1mm.
GB/T 28781-2012 Hydraulic presses — Hydraulic cylinder specifications