E43-356 · Welded/Cast Forming Dimensional Error · A steel-bridge gusset 24mm thick, 800mm hole spacing, designed spacing 800±0.3, measured 805.1 · ★★
Weld angular distortion of the gusset pushes the bolt-hole spacing 5.1mm out of tolerance, so high-strength bolts cannot pass through.
[Mechanism] Uneven shrinkage of multi-direction welds on the gusset produces angular distortion, shifting the whole hole group and pushing spacing out of tolerance.
[Calculation] Hole-spacing shift Δ≈f·L/B=2.5×800/400≈5mm (angular distortion f=2.5mm over width 400).
[Design Omission] No welding sequence or distortion control — a design defect leading to hole-spacing error.
1) Drill holes after welding and flattening;
2) Set a welding sequence from long to short welds to reduce distortion;
3) Add temporary rigid fixing to prevent angular distortion;
4) Flatten with a flattening press after welding;
5) Drill holes with a CNC drill template/jig;
6) Match-drill the hole group to keep coaxiality;
7) 100% inspect with a hole-spacing gauge;
8) Trial-fit bolts on the first article to verify.
GB/T 50205-2020 Standard for acceptance of construction quality of steel structures