Knowledge Base › Tolerance and Fit Error Case › Steam-Turbine Casing Casting Hot-Spot Shrinkage Cavity Causing Wall-Thickness Error

Steam-Turbine Casing Casting Hot-Spot Shrinkage Cavity Causing Wall-Thickness Error

E43-359 · Welded/Cast Forming Dimensional Error · A turbine casing 60mm wall at the hot spot, designed wall 60±2, measured 52 at the cavity · ★★★

Problem Description

A casting hot-spot shrinkage cavity thins the local wall by 8mm, causing leakage in the pressure test.

Root Cause

[Mechanism] At the thick-wall hot spot the metal solidifies late; inadequate feeding forms a shrinkage cavity, thinning the local wall and lowering strength.
[Calculation] Shrinkage-cavity ratio≈(V_hot-V_feed)/V≈8/60≈13%; the 8mm wall loss is 4× the tolerance of 2.
[Design Omission] No riser feeding or chill to control solidification — a design defect leading to wall-thickness error.

Corrective Solution

1) Provide a riser at the hot spot for adequate feeding;
2) Add chills to speed thick-wall solidification;
3) Optimize the gating system for even temperature;
4) Leave machining allowance on the wall to compensate;
5) Inspect for shrinkage cavities by UT;
6) Increase sand-mold compactness;
7) 100% inspect wall thickness with a thickness gauge;
8) Pressure-test the first article with no leakage.

Checklist

Reference

GB/T 6414-2017 Castings — Dimensional tolerances and machining allowance