E43-366 · Welded/Cast Forming Dimensional Error · A cast-aluminum gearbox housing 8mm wall, designed wall 8±0.5, measured 6.2 at the porosity · ★★
Shrinkage porosity in the thick aluminum wall thins the local wall by 1.8mm, causing leakage in the pressure test.
[Mechanism] Filled aluminum cools fast; at thick walls feeding is inadequate, producing shrinkage porosity and thinning the wall.
[Calculation] Porosity rate≈(8-6.2)/8=22%; the 1.8mm wall loss is 3.6× the tolerance of 0.5.
[Design Omission] No riser or chill to control solidification — a design defect leading to wall-thickness error.
1) Provide a riser at thick walls for feeding;
2) Add chills to speed solidification;
3) Optimize pouring temperature and rate;
4) Leave machining allowance on the wall;
5) X-ray inspect for porosity;
6) Improve mold venting;
7) 100% inspect wall thickness;
8) Pressure-test the first article with no leakage.
GB/T 9438-2013 Aluminum-alloy castings