E43-365 · Welded/Cast Forming Dimensional Error · A tower flange 3200mm diameter, designed flange flatness 1.0, measured post-weld 3.5 · ★★
Circumferential weld angular distortion between tower and flange pushes flange flatness 3.5mm out of tolerance and makes bolt preload uneven.
[Mechanism] Angular distortion of the thick-flange-to-shell circumferential weld warps the flange face off the theoretical plane.
[Calculation] Angular distortion f≈B·θ/2=200×tan1°/2≈1.7 (3.5mm measured after multiple passes), 3.5× the tolerance of 1.
[Design Omission] No double-sided welding or distortion control — a design defect leading to flatness error.
1) Weld the circumferential seam double-sided symmetrically to reduce angular distortion;
2) Use an anti-distortion fixture to pre-bend;
3) Machine flatness after welding;
4) Add a temporary rigid ring;
5) Control heat input;
6) Stress-relieve after welding;
7) Check flatness with a straight edge;
8) Measure first-article flatness ≤1.0mm.
GB/T 19072-2010 Wind turbine generator systems — Towers