E43-368 · Welded/Cast Forming Dimensional Error · A 1200mm cast-iron table, designed flatness 0.02, measured post-roughing distortion 0.12 · ★★★
Inadequate aging releases stress after rough machining, pushing table flatness 0.12mm out of tolerance.
[Mechanism] The casting was not adequately aged; after rough machining removes the skin, internal stress redistributes and causes distortion.
[Calculation] Distortion Δ≈σ·L²/(8Eh)=25×1200²/(8×110000×200)≈0.05 (0.12mm measured with clamping force added).
[Design Omission] No second aging or separation of rough and finish machining — a design defect leading to flatness error.
1) Thermally age ≥8h before rough machining;
2) Add a second aging step between rough and finish machining;
3) Leave allowance in rough machining;
4) Measure the datum plane before machining;
5) Low-stress fixturing;
6) Supplement with natural aging;
7) Check by scraping with a straight edge;
8) Measure first-article flatness ≤0.02mm.
GB/T 11337-2004 Flatness tolerances