Thin-Wall Shell Weld Buckling Causing Polygonal Roundness Error

E43-375 · Welded/Cast Forming Dimensional Error · A thin-wall shell 600mm diameter, 4mm wall, designed roundness 0.5, measured post-weld polygon 3 · ★★★

Problem Description

Thermal weld shrinkage buckles the thin-wall shell into a polygon, pushing roundness 3mm out of tolerance and distorting the shape.

Root Cause

[Mechanism] The thin shell has low stiffness; weld shrinkage buckles it into a polygon, pushing roundness out of tolerance.
[Calculation] Critical buckling Δ≈0.1·t·(D/t)^1.5/...≈ actual polygon 3 (thin wall, insufficient stiffness), 6× the tolerance of 0.5.
[Design Omission] No internal support or low-stress welding — a design defect leading to polygonal roundness error.

Corrective Solution

1) Use an internal support fixture during welding to hold roundness;
2) Use low current and low heat input for thin walls;
3) Weld symmetrically in segmented skip passes;
4) Round-up after welding;
5) Add temporary ring stiffeners;
6) Control the welding sequence;
7) Measure roundness with a caliper gauge;
8) Measure first-article roundness ≤0.5mm.

Checklist

Reference

GB/T 1804-2000 General tolerances — Tolerances for linear and angular dimensions without individual tolerance indications