Knowledge Base › Tolerance and Fit Error Case › Cast-Steel Bracket Heat-Treatment Distortion Causing Mounting-Hole Error

Cast-Steel Bracket Heat-Treatment Distortion Causing Mounting-Hole Error

E43-374 · Welded/Cast Forming Dimensional Error · A cast-steel bracket with 500mm mounting-hole spacing, designed 500±0.2, measured 503.1 · ★★

Problem Description

Quenching-and-tempering distortion of the bracket pushes mounting-hole spacing 3.1mm out of tolerance, so bolts cannot pass through.

Root Cause

[Mechanism] Uneven cooling in heat treatment distorts the bracket, shifting the whole mounting-hole group.
[Calculation] Hole-spacing shift Δ≈α·ΔT·L=11.5e-6×40×500≈0.23 (3.1mm measured with furnace distortion), 15× the tolerance of 0.2.
[Design Omission] No control of heat-treatment tooling or of heat-treating before drilling — a design defect leading to hole-spacing error.

Corrective Solution

1) Use distortion-control tooling in heat treatment;
2) Heat-treat first, then drill;
3) Use drill bushings to hold hole spacing;
4) Control cooling uniformity;
5) Leave allowance in rough machining;
6) Measure hole spacing on a CMM;
7)Trial assemblyBolt;
8) Measure first-article hole spacing ≤0.2mm.

Checklist

Reference

GB/T 11352-2009 Cast carbon steel castings for general engineering use