E44-986 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
No impact energy, brittle fracture, cracking
[Mechanism] The material came with no low-temperature impact-energy certificate; its actual low-temperature toughness was unknown, and it fractured brittlely at low temperature.
[Calculation] The Q245R material arrived with only room-temperature mechanical properties and no -20℃ impact data; re-test at -10℃ gave impact energy 20J, below 27J, KIC=30 at the critical point.
[Design Omission] No impact test required, no low-temperature toughness check, and no re-verification.
1) Mandate -20℃ impact (≥27J) with a report in the purchase spec, since there were no data and re-test reveals it — thus quantifying acceptance;
2) Check low-temperature impact energy (samples at design temperature +0℃, ≥27J), since missing low-temperature toughness caused fracture and the impact check assures it — thus compliant toughness;
3) Choose Q345R low-temperature grade (normalized, -20℃ qualified), since plain carbon was untested and a better steel is reliable — thus preventing brittleness;
4) Re-verify impact on delivery (3 pieces per lot), since mixed material causes fracture and re-test rejects it — thus keeping material controlled;
5) 100% inspect low-temperature-zone welds, since uninspected defects cause fracture and inspection reveals them — thus finding defects;
6) Run a -20℃ impact type test, since without testing resistance is unknown and the impact test verifies it — thus grading resistance by data;
7) Hold minimum operating temperature ≥-10℃ (limit below that), since below that it fractures and the limit avoids it — thus running to prevent fracture;
8) Write impact acceptance into the spec, since the no-impact-energy root cause was a missing purchase requirement and no re-verification — thus locking it in by specification.
GB/T 150.1-2011 Pressure vessels