E44-987 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Low allowance, thin wall, leak
[Mechanism] The corrosion allowance was set too small by rule of thumb, ignoring the actual corrosion rate; the wall thinned to failure over the service life.
[Calculation] Fluid corrosion 0.3mm/a, design life 10a, C needed 3.0mm, actual C taken 1.0mm; perforation in only 3.3a, δeff=8-3.3=4.7mm below the 7mm needed.
[Design Omission] No corrosion-rate accounting, no adequate allowance, and no periodic thickness check.
1) Recalculate C from the corrosion rate C=0.3×10=3.0mm (was 1.0mm), since an under-allowance perforates and a bigger allowance leaves wall — thus resisting corrosion;
2) Check the remaining wall (δeff≥7mm throughout), since a thin wall loses strength and the check reveals it — thus monitoring thickness;
3) Switch to corrosion-resistant 316L (corrosion rate <0.05mm/a), since carbon steel corrodes fast and a better steel eases it — thus preventing corrosion;
4) Perform periodic thickness measurement (every six months, repair if over 0.5mm loss), since thinning first shows as wall loss and can be replaced early — thus monitoring corrosion;
5) Run corrosion coupons (1a in service, weigh loss), since without measurement the rate is unknown and a coupon reveals it — thus grading the rate by data;
6) Run a hydrotest (1.25× design pressure), since thinning leaks were untested and measurement confirms no seepage — thus setting strength by data;
7) Control fluid concentration/temperature (to suppress corrosion rate), since corrosion rises with service conditions and fluid control eases it — thus running to prevent thinning;
8) Write the allowance into the calculation book, since the inadequate-allowance root cause was the missed corrosion rate and small allowance — thus locking it in at design.
GB/T 150.1-2011 Pressure vessels