E44-998 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Brittle fracture, cracking, leak
[Mechanism] At low temperature the material lacks impact toughness; a notched component fractures brittlely at normal working stress.
[Calculation] T=-40℃, using Q235B (no -40℃ impact supplied), KIC=28MPa·m^0.5, defect a=30mm, aC=28²/(1.21π×100²)=0.021m=21mm<a, 43% over.
[Design Omission] No low-temperature steel, no impact test, and no NDE.
1) Choose 16MnDR (with -40℃ impact ≥31J), since Q235B at -40℃ lacks toughness and a better steel suffices — thus preventing brittle fracture;
2) Accept -40℃ impact (≥31J per lot), since without testing toughness was unknown and the test quantifies it — thus accepting;
3) Hold minimum operating temperature ≥-30℃ (limit output below that), since below transition it gets more brittle and the limit avoids it — thus running to prevent fracture;
4) Post-weld stress-relief annealing (620℃×2h), since residual stress raises effective stress and annealing lowers it — thus raising aC;
5) 100% radiograph (Class II), since a=30mm>aC caused fracture and early rejection removes it — thus removing defects;
6) Re-verify -40℃ impact (3 pieces per heat), since there were no data and re-test verifies it — thus grading by data;
7) Hold pressure rise ≤0.3MPa/min (sudden rise damages the part), since dynamic load induces brittleness and a slow rise is steady — thus operating smoothly;
8) Write low-temperature material selection into the technical spec, since the brittle-fracture root cause was the missed 16MnDR and no impact test — thus locking it in by specification.
GB/T 150.1-2011 Pressure vessels