E44-999 · Vessel Strength and Wall-Thickness Deficiency · Nozzle · ★★★
Fillet-weld crack, leak, fracture
[Mechanism] The nozzle fillet weld was not NDE-inspected; root lack-of-fusion/undercut acted as crack sites, and internal pressure propagated them into a crack and leak.
[Calculation] Fillet leg 6mm too small, stress concentration factor 2.5, toe σ=230MPa exceeds [σ], toe crack 5mm long.
[Design Omission] No fillet-weld NDE, no reinforcement, and no welder qualification.
1) 100% MT + RT the fillet weld (no lack-of-fusion), since defects are crack sites and early rejection removes them — thus preventing cracking;
2) Add root reinforcement (R≥3δ transition), since stress concentration cracks and reinforcement lowers it — thus lowering stress;
3) Switch to a smooth transition (grind toe to R3), since a sharp toe cracks and a transition eases it — thus lowering stress;
4) Qualify welders (process covering fillet welding), since poor work makes defects and qualified welders are standard — thus weld quality;
5) Run a hydrotest (1.25× design pressure held), since cracks first show as seepage and can be repaired early — thus finding leaks;
6) Repair out-of-spec defects (grind out + reweld), since cracks first show as lines and repair restores the weld — thus removing defects;
7) Hold weld heat input ≤25kJ/cm (to prevent quench cracking), since high input cracks and controlled input is steady — thus welding steadily;
8) Write the NDE and reinforcement into the process card, since the fillet-weld crack root cause was the missed NDE and missing reinforcement — thus locking it in by process.
GB/T 150.1-2011 Pressure vessels