E44-1004 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Corrosion-fatigue crack, leak, fracture
[Mechanism] Alternating stress and corrosive medium act together, sharply dropping the fatigue limit and making cracks initiate and propagate early.
[Calculation] Δσ=90MPa, Cl- environment drops the fatigue limit from 120 to 60MPa, cracking through the 8mm wall after 2×10⁵ cycles.
[Design Omission] No stress relief, no corrosion-resistant material, and no fatigue check.
1) Remove residual stress (PWHT 620℃×2h), since Δσ stacks on residual stress and cracks, and stress relief lowers it — thus lowering Δσ;
2) Choose corrosion-resistant 316L (lower corrosion rate), since corrosion drops the limit and a better steel raises it — thus raising the fatigue limit;
3) Shot-peen the surface (0.3mm compressive layer), since a tensile surface cracks easily and compression suppresses it — thus suppressing cracking;
4) Hold fluid Cl-≤50ppm (suppress corrosion), since corrosion drops the limit and fluid control raises it — thus running to prevent cracking;
5) Run a fatigue check (Δσ≤60MPa with margin), since exceeding it cracks and the life check reveals it — thus quantifying;
6) Run a corrosion-fatigue test (CCT specimen 1000h), since without testing the limit is unknown and the test verifies it — thus grading resistance by data;
7) Keep operating conditions steady (avoid frequent starts/stops), since abrupt changes raise Δσ and steady conditions ease it — thus running to prevent cracking;
8) Write stress relief and material selection into the process card, since the corrosion-fatigue crack root cause was the missed stress relief and non-resistant material — thus locking it in by process.
GB/T 150.1-2011 Pressure vessels