E44-1005 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Hydrogen blister, bulge, crack
[Mechanism] In wet H2S, atomic hydrogen combines at inclusions/laminations into molecular hydrogen, locally pressurizing and blistering the wall.
[Calculation] H2S=30ppm, H in steel=4ppm, blister Φ25mm, blister height 3mm, propagating along laminations.
[Design Omission] No H-resistant steel, no H2S control, and no UT.
1) Choose H-resistant Q345R-HIC (Ca-treated), since plain carbon blisters easily and a better steel suppresses it — thus resisting H;
2) Hold H2S≤20ppm (desulfurize), since accumulated H blisters and fluid control suppresses it — thus suppressing H;
3) Post-weld dehydrogenation (250℃×2h), since accumulated H blisters and driving it off disperses it — thus preventing blisters;
4) Ultrasonic-test for blisters (no blister Φ≥20mm at any point), since blisters first show as protrusions and can be rejected early — thus finding blisters;
5) Run an HIC test (CLR≤15%), since without testing resistance is unknown and the H test verifies it — thus grading resistance by data;
6) Hold operating pH≥9 (suppress H release), since acidity promotes H and alkalinity eases it — thus running to prevent H;
7) Control hardness (HAZ≤200HB), since hardness cracks and controlled hardness eases it — thus lowering hardness;
8) Write H-resistance and quality control into the spec, since the hydrogen-blister root cause was the missed H-resistant steel and high H2S — thus locking it in by specification.
GB/T 150.1-2011 Pressure vessels